ATH is heat-sensitive; once temperature rises above 120–130 °C, there is risk of partial dehydration, crystal water loss, yellowing and loss of flame retardant performance. A sudden temperature spike is different from slow drift; it is triggered by an abrupt change in process condition, and the root causes are listed below, aligned with ath-mill.com ATH low-temperature grinding practice.
1. Airflow shortage / reduction of sweep air (most common)
The main way ATH systems remove heat is process sweep air.
- ID fan VFD drops, dampers close accidentally, fan slips, or fan moves into surge zone.
- Blocked baghouse filter cake, plugged cyclone, choked duct, or blocked secondary/classification air nozzles.
- Air leakage on the negative-pressure side: large inward air ingress distorts flow distribution, reduces the effective air volume passing through the grinding chamber.
With less air flow, friction heat cannot be carried away quickly, and product temperature jumps immediately.
2. Sudden feed reduction or feed interruption
When the mill runs light or empty:
- ACM: No powder cushion; rotor pins strike air and housing, mechanical friction heat rises sharply.
- VRM / ring roller mill: Material bed collapses, roller-to-metal direct contact occurs.
- Less material mass means less heat sink; the same friction energy heats a smaller amount of powder.
This is a very typical sudden spike. Bridging, rathole, sticky ATH agglomerates, feeder fault, airlock jamming can all cut off feed instantly.
3. Overloading and particle cloud over-concentration
A sudden feed surge creates a dense particle cloud inside the classifier/grinding zone:
- Inter-particle collision frequency increases dramatically.
- Air cannot penetrate the dense powder cloud, heat transfer becomes poor.
- Circulating load surges, powder recirculates many times inside the mill, residence time increases.
This often happens after hopper bridging releases a large slug of ATH.
4. Classifier wheel / labyrinth seal fouling or blockage
When ATH fines cake on classifier blades or labyrinth seal gaps:
- Internal airflow distribution changes, short-circuit flow increases.
- Classification efficiency drops, circulating load rises rapidly.
- More powder is trapped in the grinding loop, re-ground repeatedly and accumulates heat.
Seal purge air failure will accelerate this fouling.
5. Tramp hard impurities entering the grinding zone
Quartz, rock fragments or metal debris:
- Higher friction and impact energy compared with soft ATH.
- Local hot spots form instantly at the contact point.
- Often accompanied by sudden vibration and noise, together with temperature rise.
This also increases iron contamination.
6. Static and agglomeration events
A sudden static buildup or moisture excursion:
- ATH forms large agglomerates.
- Agglomerates require more energy to break, generating extra heat.
- Agglomerates may also block airflow passages locally.
Typical when process RH drifts below 30% rapidly.
7. Mechanical faults inside the mill (friction from failed components)
- Bearing degradation, lack of lubrication, bearing seizure starting.
- Rubbing between rotating and stationary parts: classifier wheel touching housing, rotor scrape, roller seal failure.
- Loose liner, loose pin, deformed component after a previous choke.
This type of temperature rise is usually accompanied by rising vibration and abnormal bearing temperature.
8. Hot air source intrusion (less common but possible)
- If upstream flash dryer control malfunctions, overheated dry ATH feed enters the mill.
- Leakage of hot flue gas or hot oil heat tracing into the process air stream.
9. Fan and exhaust system reversal of heat
When the baghouse is heavily loaded and differential pressure spikes, hot exhaust cannot be discharged normally; heat backs up into the mill circuit.
How to quickly distinguish the root cause
- If temperature rises together with low motor current: feed loss / empty bed / airflow reduction.
- If temperature rises together with high motor current: overload, high circulating load, agglomerates, tramp silica.
- If temperature rises plus vibration + abnormal noise: metal rubbing, tramp contaminants, bearing fault.
- If temperature rises slowly after startup and spikes after several hours: fouling of classifier blades / cyclone / bags.
Immediate corrective actions for ATH
- First check feed status: confirm feeder, airlock, hopper bridging. Restore stable feed or reduce feed rate.
- Check fan current, VFD setpoint, differential pressure of baghouse and cyclone to confirm airflow.
- Check labyrinth seal purge air, clean classifier wheel if fouling is visible.
- Stop feeding if metal rubbing / tramp material is suspected to avoid permanent damage and ATH discoloration.
- Keep process humidity stable at 40–50% to prevent agglomeration.
Once temperature exceeds 130–140 °C, ATH begins to lose crystal water gradually. Even if you cool it down later, the flame retardancy and whiteness cannot be recovered for that batch. High temperature also increases static spark risk and ATEX hazard.